Wrinkling and Cracking

Causes and Solutions for Tube Wrinkling

Causes of Wrinkling

This is usually on the inner portion of a curve (the inside radius). Wrinkling occurs. During bending, the material in this region is subjected to tangential compressive stress. Once the compressive stress is over the yield limit of the material and there is insufficient radial and tangential support, the material will buckle and swell inward creating ripples or folds.

1.An incorrect mandrel location The mandrel head is too distant from the tangent point of the bend or the lead is not enough, and is unable to provide sufficient support for the tube wall about to undergo compressive deformation.
2.Excessive tool clearance: The clearance between the tube outer diameter and the bending die, wiper die or clamp die is too loose, allowing the tube wall to move freely under compression.
3.Incompatible mandrel segments or structure: In the case of thin-walled tubes or tubes with a tiny bending radius (small $R/D$), the mandrel does not have the sufficient rigidity or segments to match the deformation zone.
4.Wall too thin The wall of the tube itself is too large and too thin (diameter too large and wall too thin), hence the resistance to self-buckling can be quite low.

Solutions for Wrinkling

Optimize mandrel lead (extension). Adjust the mandrel position so that the mandrel tip is closer to the tangent point of the bending angle (usually controlled within a very small range or adjusted to an overreach state according to the tube diameter) to guarantee that the internal support is provided at the exact moment of deformation.

 

Reduce tool clearance : make sure that the depth of the die groove is precisely equal to the diameter of the tube to restrict lateral movement of the tube wall.

 

Use a multi-ball flexible mandrel: Increase the number of articulated joints on the mandrel (packed close ball joints) and provide adequate lubrication so friction is minimized and that there is continuous support of the inner wall.

Deformation Type Main Occurrence Area Core Trigger Key Solutions
Wrinkling Inner radius side of the tube Excessive tangential compressive stress, delayed internal support, loose clearance Shorten mandrel lead, install wiper die, increase mandrel ball joint density

Phone: +86 189 6229 6262
Website: www.hsformer.com
Email: heshun@heshunjx.com

Best Regards,

The Team at Zhangjiagang Heshun Machinery Co., Ltd.